and flux mineral were researched systematically. Finally it is to ascertain that the
available C3S is 30%~40% and C2S is 40%~50%. The optimum C3A is specified
under 4% and C4AF is in the scope of 15%~19%.
A certain chemical shrinkage occurs to cause concrete self-constriction by
cement hydration which is seriously critical in low cementitious ratio concrete. The
crack risk will easily incur if volume shrinkage and procedure of temperature
decrease overlap together. P.MH cement with 3.5%~5.0% MgO was adopted in the
Three Gorges Project to improve crack resistance such that the shrinkage can
be compensated effectively with well result and concrete was in micro expansion
mode while temperature decreased[18]. In the research of P.LH cement, concrete
test in low MgO has ever been conducted and it is resulted that concrete volume
constriction became bigger. While other restraints unchanged, concrete volume
constriction with P.LH in low MgO obviously became smaller and presented micro
expansion. In accordance with relevant research result, concrete volume mixed
with P.LH cement in 4.67% MgO is in micro expansion mode [13], but negative
influence to cement strength becomes great while MgO over 5%[14]. Thus MgO in
P.LH cement clinker shall be in the scope of 4.0%~5.0%.
The compressive strength and hydration heat are affected seriously by
cement fineness(Fig.1) referring to a great deal of research result. The finer the
cement is, the larger the surface area will be, the faster the hydration reacts, the
quicker the concrete condenses and hardens to cause high 28d compressive
strength and more 3d early hydration heat. Simultaneously not only will the cement
cost and water be increased, and more constricted, but also more energy will be
needed while milled more finely. The research by the US Bureau of Reclamation
indicates concrete frost resistance will become worse while cement was milled
finely[14]. The relationship between cement surface area and RCC frost resistance
by Chinese scholars makes clear it is helpful to improve concrete frost resistance
while cement surface area reduced[15]. Surface area of the special P.LH cement
applied in ultra arch dam shall be within 340m2/kg in overall consideration of the
influence to cement strength and hydration heat, etc.
Fig. 1 Effect of specific surface area on compression strength and hydration heat
of low heat Portland cement
In accordance with the research above, the mineral composition and
chemical components to produce special P.LH cement in ultra arch dam are shown
1681
Book of Full Papers
Symposium Hydro Engineering
- Titel
- Book of Full Papers
- Untertitel
- Symposium Hydro Engineering
- Autor
- Gerald Zenz
- Verlag
- Verlag der Technischen Universität Graz
- Ort
- Graz
- Datum
- 2018
- Sprache
- englisch
- Lizenz
- CC BY-NC-ND 4.0
- ISBN
- 978-3-85125-620-8
- Abmessungen
- 20.9 x 29.6 cm
- Seiten
- 2724
- Schlagwörter
- Hydro, Engineering, Climate Changes
- Kategorien
- International
- Naturwissenschaften Physik
- Technik